    摘要进入高速列车时代以来,铁路客运量的需求日益增加,列车速度性能的要求也不断提高,高强度铝合金材料在高速列车车体上得到了广泛的应用。然而铝合金材料在潮湿气体中具有抗应力腐蚀开裂(SCC)敏感性,所以有必要对其抗SCC性能进行研究。25290
        本文通过对高速列车用6N01铝合金的应力腐蚀性能的研究,结合实验室条件,进行了自加载悬臂梁试验以及三点加载应力腐蚀试验,测量6N01铝合金应力腐蚀强度因子和裂纹扩展速率,研究应力腐蚀过程及机理,比较5、6、7mm不同厚度的铝合金板材的抗应力腐蚀性能以及T4、T5态的铝合金板材应力腐蚀敏感性的差异。
        经试验研究发现,在实验条件下 6N01铝合金板材会发生应力腐蚀现象,在三点加载作用下受拉应力作用的表面氧化膜首先被破坏,并在表面产生点蚀和晶间腐蚀,随着晶粒慢慢剥蚀表面产生了腐蚀坑,腐蚀坑之间逐渐连成片并出现裂纹。测量计算得到6N01铝合金临界应力强度因子为4.9-5.6Mpa左右,裂纹扩展速率约为4.5*10-3mm/h。在一定厚度范围内,5mm的铝合金板材腐蚀速率较慢,腐蚀程度较低,其抗应力腐蚀敏感性较6mm和7mm板材更低。T4状态的铝合金板材比T5状态的的应力腐蚀敏感性更低。
    关键词  6N01铝合金   应力腐蚀   KISCC     三点加载   裂纹扩展速率
    毕业论文设计说明书外文摘要
    Title Study of Stress Corrosion Cracking of High-strength aluminum alloy                                                          
    Abstract
    Enter into the high-speed train era, the demand of railway passenger traffic
    have increased quickly,the need of passenger train speed performance improved too,So the high-strength aluminum alloy in high-speed train body has been widely used.However,there are SCC susceptibility of aluminum alloy material in the wet gas, so it is necessary to study its resistance to SCC.
    This topic through 6N01 aluminum alloy used for high-speed trains to inquiry stress corrosion, Combined with laboratory conditions,Carried out the self-loading izod test and three point loading stress corrosion test.Measured the intensity factor and stress corrosion crack growth rate of 6N01 aluminum,researched the stress corrosion mechanism,compared the different thicknesses of aluminum alloy sheet 5,6,7mm resistance to stress corrosion and T4, T5 state aluminum plate stress corrosion sensitivity of difference.
    Experimental research has found that 6N01 aluminum alloy is sensitive to stress corrosion,surface oxide film under tensile stress in three-point loading effects are first destroyed and pitting and corrosion on the surface of the grain.With the grain slowly eroded surface corrosion pits, the gradual emergence of microcracks between corrosion pits.6N01 aluminum measure calculated critical stress intensity factor of about 5Mpa, the crack growth rate is about 4.5E-3.Within a certain range of thickness aluminum sheet thinner the better resistance to stress corrosion, stress corrosion resistance of aluminum alloy sheet can be better than 5mm and 7mm of 6mm. Aluminum alloy sheet T5 T4 state than the state more resistant to corrosion.
    Keywords  6N01 aluminum   Stress corrosion    KISCC   Three loaded    Crack growth rate
    目   次
    1  引言    1
    1.1  高速列车的车体材料    1
    1.2  铝合金概论    2
    1.2.1  变形铝合金的分类    2
  1. 上一篇:Hummers石墨烯添加量对镍基复合镀层摩擦学性能的影响
  2. 下一篇:复合钎料连接铝基复合材料工艺
  1. 微量元素对钛铝合金微观组织的影响

  2. 厚板铝合金激光焊接工艺性能研究

  3. 高强铝合金螺柱感应+拉弧...

  4. 高强铝合金中厚板双脉冲...

  5. 6mm中厚板5083高强铝合金双...

  6. 高强铝合金多层结构箔片...

  7. 铝合金螺旋管连续生产T...

  8. java+mysql车辆管理系统的设计+源代码

  9. 中考体育项目与体育教学合理结合的研究

  10. 乳业同业并购式全产业链...

  11. 十二层带中心支撑钢结构...

  12. 当代大学生慈善意识研究+文献综述

  13. 杂拟谷盗体内共生菌沃尔...

  14. 酸性水汽提装置总汽提塔设计+CAD图纸

  15. 电站锅炉暖风器设计任务书

  16. 大众媒体对公共政策制定的影响

  17. 河岸冲刷和泥沙淤积的监测国内外研究现状

  

About

751论文网手机版...

主页:http://www.751com.cn

关闭返回